CEE 200X photoresist spinner 2
| CEE 200X photoresist spinner 2 | |
|---|---|
| Equipment Details | |
| Technology | Lithography |
| Materials Restriction | General |
| Material Processed |
SPR 220 (3.0) 1813 SPR 955 (0.9) |
| Sample Size | pieces up to 6" wafers |
| Equipment Manual | |
| Overview | System Overview |
| Operating Procedure | SOP |
| Supported Processes | Supported Processes |
| Maintenance | Maintenance |
The CEE 200X photoresist spinner 2 is a fully programmable, automatic dispense, photoresist spinner located in 1440C. This tool has multiple chucks for 4" and 6" wafers, as well as pieces up to 2". It has automatic photoresist dispensers, but can also accommodate manual dispensing.
Contents
Announcements
SPR 955 has been added to this tool.
Capabilities
Equipped Photoresists: SPR 220 (3.0), 1813, SPR 955 (0.9)
System overview
Hardware details
- Up to 6K rpm spin rates
- Hot plate up to 200°C
- Photoresist is dispensed automatically with an equipped photoresist or through an EFD tube.
Substrate requirements
- 1x1 cm pieces up to 6" wafers
- No substrate material requirements
- Available Chucks
- 6" Chuck (Ø 3.75")
- 4" Chuck (Ø 2.25")
- Large Piece Chuck (Ø 0.75")
- Small Piece Chuck (Ø 0.25" - chuck ; Ø 0.375" - O-ring)
Material restrictions
The CEE 200X photoresist spinner 2 is designated as a General class tool. Below is a list of approved materials for the tool. Approved means the material is allowed in the tool under normal circumstances. If a material is not listed, please create a helpdesk ticket or email info@lnf.umich.edu for any material requests or questions.
Supported processes
The CEE 200X has recipes in 1000 rpm increments from 1000 to 5000 rpm for each of the equipped photoresists as well as for manual dispensed photoresists. There are recipes for pieces larger than 15 mm, 100 mm wafers and 150 mm wafers. The primary difference between theses recipes is how much photoresist is dispensed.
Details for the available recipes can be found in the following tables. These include average thicknesses expected using the automatic dispense recipes as well as examples for bake times, exposure values, and develop times. These parameters may vary for individual processes.
This section's factual accuracy is disputed. |
| SPR 220 (3.0) | ||||||
|---|---|---|---|---|---|---|
| Spin Speed | Thickness | Softbake | Stepper Exposure | Contact Aligner Exposure | Post Exposure Bake | Puddle Develop Time |
| 1000 rpm | 4.6 µm | 115°C for 90 sec | 0.35 sec | ? | 115°C for 90 sec | AZ 726 DP 70-70 |
| 2000 rpm | 3.2 µm | 115°C for 90 sec | 0.33 sec | ? | 115°C for 90 sec | AZ 726 DP 60-60 |
| 3000 rpm | 2.5 µm | 115°C for 90 sec | 0.32 sec | ? | 115°C for 90 sec | AZ 726 DP 40-40 |
| 4000 rpm | 2.2 µm | 115°C for 90 sec | 0.25 sec | ? | 115°C for 90 sec | AZ 726 DP 60 |
| 5000 rpm | 1.9 µm | 115°C for 90 sec | 0.25 sec | ? | 115°C for 90 sec | AZ 726 DP 60 |
| 1813 | ||||||
|---|---|---|---|---|---|---|
| Spin Speed | Thickness | Softbake | Stepper Exposure | Contact Aligner Exposure | Post Exposure Bake | Puddle Develop Time |
| 1000 rpm | 2.8 µm | 115°C for 60 sec | ? | ? | None | ? |
| 2000 rpm | 2.0 µm | 115°C for 60 sec | .35 | ? | None | AZ 726 SP 60 |
| 3000 rpm | 1.6 µm | 115°C for 60 sec | ? | ? | None | ? |
| 4000 rpm | 1.4 µm | 115°C for 60 sec | ? | ? | None | AZ 726 SP 30 |
| 5000 rpm | 1.2 µm | 115°C for 60 sec | ? | ? | None | ? |
Standard operating procedure
Checkout procedure
- Complete a Lithography training session. If you have already completed this for another tool, you do not need to complete it again.
- Practice on the tool with your mentor.
- Read through the SOP above.
- Accurately complete the checkout quiz. You may retake as necessary until all answers are correct.
- Schedule a time for a checkout:
- Find an available time for checkout here.
- Verify that the tool is available in the LNF Online Services at the time you are requesting.
- After confirmation that the event is scheduled in Calendly, invite the staff member assigned to your event to a Staff Support reservation at that time.
- Create a helpdesk ticket for final confirmation of your checkout appointment.
- Authorization will be provided pending demonstration of proper tool use in the presence of a tool engineer.
Maintenance
Photoresist levels are checked several times a week and replaced when low. The bowls and chucks are cleaned each week during lab clean.
User authorized maintenance
In the event of a power bump, users may run the startup/shutdown procedure.