LAM 9400/Processes/LNF Ti thin
Jump to navigation
Jump to search
About this Process | |
---|---|
Process Details | |
Equipment | LAM 9400 |
Technology | RIE |
Material | Titanium |
Mask Materials | PR |
Gases Used | SF6, C4F8, Ar |
Date Created | June 2018 |
LNF_Ti_thin is for etching very thin layers of Ti (10-20nm) with a PMMA mask.
Etch Rates
These were in a 90-180 sec long etch on 1cm pieces with a 6" SiO2 carrier.
- Titanium - 6.9 nm/min
- PMMA - 9-11 nm/min
- ZEP - ~ 4.3-8 nm/min
- SPR 220 - 9 nm/min
- SiO2 - 4.7 nm/min
Parameters
Parameter | Main Etch |
---|---|
Pressure | 30 mTorr |
TCP Power | 200 W |
Bias Power | 30 W |
SF6 Flow | 5 sccm |
C4F8 Flow | 45 sccm |
Ar Flow | 45 sccm |