LAM 9400/Processes/LNF Poly

141 bytes added, 1 year ago
no edit summary
[[Category:Processes]] [[Category:RIE]]
LNF_Poly is designed for etching si [[Silicon|Si]] and polysilicon [[Polysilicon]] in the LAM 9400. This recipe is currently under development produces a very vertical sidewall angle and will replace poly_etch_2 as it does not have the same stability problemshas a high selectively to oxide (~18:1).
==Etch Rates==
* Polysilicon - 2340 Å/min (blanket 150mm poly)*Si - 2800 Å/min(<10% open area)
*SPR 220 (3.0) - 275 Å/min
*SiO<sub>2</sub> - 150 Å/min
==Limitations==
To remove the photoresist a ~20 sec dip in 100:1 HF is necessary before nanostrip.