===Hardware Details===
*Turbo-pumped/Water-pumped (high temp cryo that acts as a water trap,) loadlocked sputtering tool. Base pressures in the 10-7, 10-8 range
*10 KW AC power supply that runs 5-7KW power across a dual Al target source
*RF bias on wafer holding platen to control surface characteristics.thru Ar and N2 bombardment*Backside lamp heating*100 50 sccm N<sub>2</sub> and 20sccm Ar and 20sccm O2 flow meters.
*Handler for 6" wafers, carrier for 4" wafers.
===Substrate Requirements===
*'''4” and 6" wafers only'''
*The process heats the wafer considerably (~500°C or more) with heavy ion bombardment so no organics or low temperature films are allowed in the tool.
*The process only produces piezoelectric AlN films on certain materials (specifically blanket undoped or low-doped Si, SiO<sub>2</sub> and patterned Mo, Pt, Al.)
**Thickness data collected by users and staff in the logbook will be used to adjust and improve the accuracy of the target file.
<gallery mode="packed-hover" heights="500px400px">
File:Endeavor_M1_Thickness_Response.jpeg
</gallery>
 
====Stress Adjustment Unit====
*The stress adjustment unit is used to adjust change the resistance in a capacitance/resistance path circuit to ground of the chamber.
**Users can adjust the dial before their runs.
**Typically adjustments below 25 will lead to plasma instability issues so the vendor does not recommend going below that point.
**The response for 1um films is below. Thicker films (1.5-2.5um) usually have less compressive stress. Thinner films will have more compressive stress.
<gallery mode="packed-hover" heights="500px450px">
File:Endeavor_M1_SAU_Response.jpeg
</gallery>
 
 
====AlN Hysteresis:====
==Checkout Procedure==
<!-- Describe the checkout procedure for the tool. For example: -->
*Read through this page and the Standard Operating Procedure above.
*Create a [http://ssel-sched.eecs.umich.edu/sselScheduler/ResourceContact.aspx?tabindex=3&path=0:0:0:{{#var:toolid}} Helpdesk Ticket] requesting training.
*A tool engineer will schedule a time for initial training.
==Maintenance==
There is no maintenance allowed by users of this tool.
===Power Bump Recovery===
The only maintenance that users are allowed *In case of a power bump, nothing on the tool is time-critical or will lead to perform is power interruption recoverytool damage. *Follow The tool power up requires multiple steps and some system checks in the service aisle.Therefore, for power bump part of the [https://docsrecovery, please contact staff and do not attempt to unload any wafers.google.com/document/d/1r6gMJ77YZu0C75i8ZLnxSTcw9DgRo8nZcWkcLZwYRXg/preview AMS 2003 AlN Startup and Shutdown Procedure]