<!-- Make sure to add any other relevant categories -->{{#ifeq: {{NAMESPACE}} | Template | | [[Category:Processes]]}}{{warning|This page has not been released yet.}}{{Infobox process
|image =
|caption =
|authors =
}}
'''{{SUBPAGENAME}}''' (previously known as '''LNF si thinning etch - slow 1''') is an SF<sub>6</sub> based process intended for isotropic thinning of Si wafers for device release.
==Procedure==
|-
| Silicon dioxide
| ? 240 Å/min| ?7%
|-
| Silicon nitride
| ?700 Å/min| ?2%|-| Low stress nitride| 590 Å/min| 2%
|-
| SPR 220