{{#ifeq: {{NAMESPACE}} | Template | | [[Category:Processes]]}}{{warning|This page has not been released yet.}}{{Infobox process
|image =
|caption =
|technology = Lithography
|material =
|mask =
|chemicals = AZ 12XT, AZ 726
|gases = |created = 10/19/2021
|modified =
|authors =
}}
{{#allow-groups:user}}Az AZ 12XT is a chemical enhanced positive tone photo resist (PR). In a chemical enhanced PR the exposure step creates a latent image and a week acid in the PR. The chemical reaction that makes the PR soluble in developer happens during the post exposure bake (PEB). This makes the length and temperature of the PEB extremely important. One of the advantages of the chemical enhance resits for thick resist is that it eliminate the waiting steps. The resist holds up well in RIE, DRIE, wet etching and plating. We have seen some PR cracking after gold platting but have had no plating in the cracks or peeling of the PR.
Users should note that this is not a DNQ resist and is not compatible with the image reversal process used in the [[Image Reversal Oven|YES-310TA]].
 
==Announcements==
*On 1/18/22 our contact aligner lamps are being re calibrated. This may increase the required exposure by up to 22%. This page will be updated after we have time verify the new exposure times.
 
==Procedure==
===for 10-17um 25um layers===
* HMDS in YES Image Reversal Oven
**For Plating or glass RIE etching set the oven temp to 140°C. You need to allow 40 minutes each for the oven to heat and cool.
**RIE and wet etching can us HMDS applied at 90°C
*Spin AZ 12xt
**When dispensing the AZ 12xt try to spread the puddle around as you dispense. You can get good even coverage with less resist this way.
**AZ 12xt is a high viscosity resist and will create stringers or cotton candy when spun.
**For 4 inch or larger samples you need to knock down the stringers with a swab or acetone between samples.
*Softbake
** 2-4K 3 minutes on a 110°C hotplate with the lid lowered
**1K 4 minutes on a 110°C hotplate with the lid lowered
*Exposure(see characterization data below)
**10-17um layers
***Contact Alingers Aligners 12-16 sec***Stepper 0.22-0.24 sec, Focus -30 to :-50
**>17um
***Contact Alingers Aligners 20-24sec*Post Exposure Bake
** For 3 and 4k spins - 1 minute on a 90° hotplate with the lid lowered
**For a 2K spin - 1.5 minutes on a 90° hotplate with the lid lowered
*Develop on the CEE Develop stations using 726 DP 60-60
*Hard Bake
**For wet etching or platting Wet processing: hard bake at 110°C for 1 minute
*Removal
**For thickness <17um spins removal as normalIf wafers have been through a plasma you MUST start with a Oxygen ash to remove most the pr. (ash, You can follow with PRS-2000, or nanostrip)**For thickness >17um***If wafer have been through any other process you can use Oxygen plasma, PRS-2000 at 60°C for 10-15 minutes, or***Ash at temp lower than 100°C to break through RIE hardened layer***PRS-2000 after ash to remove most of PRnanostrip.
==Characterization==
===Characterization Matrices===
*Contact Aligners: Exposure time vs Spin Speed on Contact Aligners
[[File:Az12xt 2-4K crosssections.jpg|500px]]
*Contact Aligner: 1K spin, Softbake and PEB tests[[file:AZ 12xt, 1k spin SB and PEB tests.jpg|500px]] *Contact Aligner: Exposure time on Contact Aligners vs Development time. 1K spin CEE 100.
[[File:1k spin cross sections.jpg|500px]]
 
*1K Spin, Softbake and PEB tests
[[file:AZ 12xt, 1k spin SB and PEB tests.jpg|500px]]
*Exposure time vs Focus on Stepper
[[File:EXPO cross section AZ12xt.jpeg|500px]]
===Wet EtchProcess Test===*Wet Etch
[[File:Az12xt 10min BHF etch.jpg|500px]]
 
*DRIE
[[File:AZ12xt DRIE.jpg|500px]]
 
*Step Coverage
[[File:Az12xt stepcoverage.jpg|300px]]
==Data Sheets==
* [https://drive.google.com/file/d/1JzyiG9o0T74NMCGicedBsqQanjQH4jT2/view?usp=sharing| Technical Data Sheet]
* [https://drive.google.com/file/d/13p2-yEuNxjgP3S_66dVDvDZqnIE6TTUH/view?usp=sharing| Safety Data Sheet]
LabUser, OnlineAccess, PhysicalAccess, Staff, StoreManager, StoreUser
1,254

edits

Navigation menu