Difference between revisions of "LAM 9400/Processes/LNF Al2O3"

From LNF Wiki
Jump to navigation Jump to search
(Created page with "<!-- Make sure to add any other relevant categories --> {{Infobox process |technology = RIE |material = Al<sub>2</sub>O<sub>3</sub> |mask = Photoresist, SiO<sub>2</sub> |gases...")
 
 
(2 intermediate revisions by the same user not shown)
Line 5: Line 5:
 
|mask = Photoresist, SiO<sub>2</sub>
 
|mask = Photoresist, SiO<sub>2</sub>
 
|gases = BCl<sub>3</sub>, HBr
 
|gases = BCl<sub>3</sub>, HBr
|modified =
+
|created = December 2020
 
|authors = Shawn Wright
 
|authors = Shawn Wright
 
}}
 
}}
Line 11: Line 11:
 
[[Category:RIE]]
 
[[Category:RIE]]
  
This is the breakthrough step from LNF_Aluminum.
+
This is intended for etching Al<sub>2</sub>O<sub>3</sub>, and is the same as the breakthrough step in LNF_Aluminum.
  
 
==Etch Rates==
 
==Etch Rates==
Line 17: Line 17:
  
 
===Main Etch===
 
===Main Etch===
*ALD Al2O3:  28 nm/min
+
*ALD Al<sub>2</sub>O<sub>3</sub>:  28 nm/min
  
 
*SPR: 29.6 nm/min
 
*SPR: 29.6 nm/min
 
*PMMA: 73.4 nm/min
 
*PMMA: 73.4 nm/min
 
*ZEP: 49.4 nm/min
 
*ZEP: 49.4 nm/min
*SiO2: 48.4 nm/min
+
*SiO<sub>2</sub>: 48.4 nm/min
 
*GaN (N-Polar): 18.7 nm/min
 
*GaN (N-Polar): 18.7 nm/min
 
*Aluminum:  88 nm/min
 
*Aluminum:  88 nm/min

Latest revision as of 12:45, 15 December 2020


About this Process
Process Details
Equipment LAM 9400
Technology RIE
Material Al2O3
Mask Materials Photoresist, SiO2
Gases Used BCl3, HBr
Date Created December 2020
Authored By Shawn Wright

This is intended for etching Al2O3, and is the same as the breakthrough step in LNF_Aluminum.

Etch Rates

These were measured using 1cm pieces on a 6" Si carrier.

Main Etch

  • ALD Al2O3: 28 nm/min
  • SPR: 29.6 nm/min
  • PMMA: 73.4 nm/min
  • ZEP: 49.4 nm/min
  • SiO2: 48.4 nm/min
  • GaN (N-Polar): 18.7 nm/min
  • Aluminum: 88 nm/min

Parameters

Parameter Main Etch
Pressure 5 mTorr
TCP Power 600 W
Bias Power 50 W
HBr Flow 25 sccm
BCl3 Flow 25 sccm
Time Variable