About this Process
Process Details
Equipment LAM 9400
Technology RIE
Material Aluminum
Mask Materials PR
Gases Used BCl3, HBr
Date Created November 2018
Authored By Ashley Jian Shawn Wright

This is a fast anisotropic aluminum etch.

Etch Rates

Main Etch

These were measured using 1cm pieces on a 6" Si carrier.

  • Aluminum: 536 nm/min
  • ALD Al2O3: 11 nm/min (49:1)
  • SPR: 41 nm/min (13:1)
  • SiO2: 36 nm/min (15:1)
  • PMMA: 36 nm/min (15:1)
  • ZEP: 29 nm/min (18:1)


Break Through

The breakthrough step is typically set to ~10 seconds, or enough time to get through any native oxide on the aluminum.

  • Aluminum: 88 nm/min
  • ALD Al2O3: 28 nm/min
  • SPR: 29.6 nm/min
  • SiO2: 48.4 nm/min
  • PMMA: 73.4 nm/min
  • ZEP: 49.4 nm/min




Parameters

Parameter Break Through Main Etch
Pressure 5 mTorr 20 mTorr
TCP Power 600 W 600 W
Bias Power 50 W 50 W
HBr Flow 25 sccm 40 sccm
BCl3 Flow 25 sccm 10 sccm
Time 10 sec (typ) Variable