This recipe is designed to etch HfO2. Since Hf byproducts may not be effectively removed by the standard waferless autoclean we require a post etch process to be run to generate SiCl4 which is effective at cleaning Hf. The recipe "Wafer_Clean_SiCl4" needs to be run on a blank Si wafer for 5 min after etching HfO2 in this process.

About this Process
Process Details
Equipment LAM 9400
Technology RIE
Material HfO2
Mask Materials Photoresist
Gases Used BCl3
Date Created October 2021
Authored By Shawn Wright, Subhajit Mohanty
This process requires more than the standard chamber clean.


Contents

Etch Rates

These were measured using 1cm pieces on a 6" Si carrier.

Main Etch

  • HfO2 (250°C deposition): 29 nm/min
  • HfO2 (250°C deposition, annealed): 21 nm/min
  • GaN: 2.2 nm/min (13:1)
  • SPR 955:
  • ZEP:
  • PMMA:
  • SiO2:



Parameters

Parameter Main Etch
Pressure 10 mTorr
TCP Power 400 W
Bias Power 20 W
Vpk-pk ~34 V
BCl3 Flow 30 sccm
Time < 5 min

References

  1. Ramos, R., G. Cunge, and O. Joubert. "Plasma reactor dry cleaning strategy after TiN, TaN and Hf O 2 etching processes." Journal of Vacuum Science & Technology B: Microelectronics and Nanometer Structures Processing, Measurement, and Phenomena 26.1 (2008): 181-188.