Revision as of 11:47, 8 February 2016
About this Process | |
---|---|
Process Details | |
Equipment | LAM 9400 |
Technology | RIE |
Material | Poly |
Mask Materials | PR |
Gases Used | HBr, He |
Date Created | 2016 |
LNF_Poly is designed for etching si and polysilicon in the LAM 9400. This recipe is currently under development and will replace poly_etch_2 as it does not have the same stability problems.
Etch Rates
- Si - 2800 Å/min
- SPR 220 (3.0) - 275 Å/min
- SiO2 - 150 Å/min
{#widget:Iframe |url=https://docs.google.com/spreadsheets/d/1fMQ3FPo6sf2o-e0B2FYGRTN6iBklOu8UjS5TBbYDg70/pubchart?oid=1633184043&format=interactive |width=600 |height=400 |border=0 }
Parameters
Parameter | Breakthrough | Main Etch |
---|---|---|
Time | 10 sec | variable |
Pressure | 5 mTorr | 30 mTorr |
TCP Power | 300 W | 600 W |
Bias Power | 100 W | 90 W |
Cl2 Flow | 60 sccm | 0 sccm |
HBr Flow | 0 sccm | 100 sccm |
He Flow | 0 sccm | 100 sccm |