− | LNF_Poly is designed for etching [[Silicon|Si]] and [[Polysilicon]] in the LAM 9400. This recipe produces a very vertical sidewall angle and has a high selectively to oxide (~18:1). | + | LNF_Poly is designed for etching [[Silicon|Si]] and [[Polysilicon]] in the LAM 9400. This recipe produces a very vertical sidewall angle and has a high selectively to oxide (~18:1). This process requires a large amount of exposed silicon in order to stabilize, so a Si carrier wafer is required. |
==Etch Rates== | ==Etch Rates== |
Revision as of 17:02, 26 November 2019
About this Process | |
---|---|
Process Details | |
Equipment | LAM 9400 |
Technology | RIE |
Material | Poly |
Mask Materials | PR |
Gases Used | HBr, He |
Date Created | 2016 |
LNF_Poly is designed for etching Si and Polysilicon in the LAM 9400. This recipe produces a very vertical sidewall angle and has a high selectively to oxide (~18:1). This process requires a large amount of exposed silicon in order to stabilize, so a Si carrier wafer is required.
Etch Rates
- Polysilicon - 2340 Å/min (blanket 150mm poly)
- Si - 2800 Å/min (<10% open area)
- SPR 220 (3.0) - 275 Å/min
- SiO2 - 150 Å/min
Parameters
Parameter | Breakthrough | Main Etch |
---|---|---|
Time | 10 sec | variable |
Pressure | 5 mTorr | 30 mTorr |
TCP Power | 300 W | 600 W |
Bias Power | 100 W | 90 W |
Cl2 Flow | 60 sccm | 0 sccm |
HBr Flow | 0 sccm | 100 sccm |
He Flow | 0 sccm | 100 sccm |
Sidewall Profile
- Nearly a 90 degree sidewall angle
Limitations
To remove the photoresist a ~20 sec dip in 100:1 HF is necessary before nanostrip.