LAM 9400/Processes/LNF Poly

From LNF Wiki
Jump to navigation Jump to search


About this Process
Process Details
Equipment LAM 9400
Technology RIE
Material Poly
Mask Materials PR
Gases Used HBr, He
Date Created 2016

LNF_Poly is designed for etching Si and Polysilicon in the LAM 9400. This recipe produces a very vertical sidewall angle and has a high selectively to oxide (~18:1).

Etch Rates

  • Polysilicon - 2340 Å/min (blanket 150mm poly)
  • Si - 2800 Å/min (<10% open area)
  • SPR 220 (3.0) - 275 Å/min
  • SiO2 - 150 Å/min

Parameters

Parameter Breakthrough Main Etch
Time 10 sec variable
Pressure 5 mTorr 30 mTorr
TCP Power 300 W 600 W
Bias Power 100 W 90 W
Cl2 Flow 60 sccm 0 sccm
HBr Flow 0 sccm 100 sccm
He Flow 0 sccm 100 sccm

Sidewall Profile

  • Nearly a 90 degree sidewall angle

Limitations

To remove the photoresist a ~20 sec dip in 100:1 HF is necessary before nanostrip.