Difference between revisions of "PMMA A4 4krpm"
Jump to navigation
Jump to search
Line 29: | Line 29: | ||
Exposure is performed on the [[JEOL JBX-6300FS Electron Beam Lithography System|JEOL E-Beam]]. Exposure dosage will depend on the materials on the sample and feature size. The standard exposure on [[silicon]] is {{em|650{{nbsp}}μC/cm<sup>2</sup>}}. For an oxide film, this can be increased to {{em|675{{nbsp}}μC/cm<sup>2</sup>}}. For large or varied features, the tool supports [[proximity correction]]. | Exposure is performed on the [[JEOL JBX-6300FS Electron Beam Lithography System|JEOL E-Beam]]. Exposure dosage will depend on the materials on the sample and feature size. The standard exposure on [[silicon]] is {{em|650{{nbsp}}μC/cm<sup>2</sup>}}. For an oxide film, this can be increased to {{em|675{{nbsp}}μC/cm<sup>2</sup>}}. For large or varied features, the tool supports [[proximity correction]]. | ||
− | {{note|For assistance characterizing exposure dose, please create a [ | + | <!--{{note|For assistance characterizing exposure dose, please create a [https://ssel-sched.eecs.umich.edu/sselScheduler/ResourceContact.aspx?tabindex=3&path=0:0:0:52011 helpdesk ticket].}}--> |
+ | {{note|For assistance characterizing exposure dose, please create a helpdesk ticket.}} | ||
===Development=== | ===Development=== |
Revision as of 10:09, 17 May 2016
This page has not been released yet. |
About this Process | |
---|---|
Process Details | |
Equipment | PMMA A4 4krpm |
Technology | Electron beam lithography |
Material | PMMA |
Chemicals Used | MIBK |
Date Created | 5/16/2016 |
Authored By | Kevin Owen |
PMMA A4 4krpm is a standard process using PMMA A4 to produce a 200 nm thick mask with electron beam lithography.
Contents
Procedure
Photoresist spin and soft bake
The photoresist spin and bake should be performed at the E-Beam Spinner/Hot-Plate Bench.
- Start the bench and let the hot plate heat to 180°C
- Mount the correct chuck, depending on sample size, onto the spinner
- Load the 4krpm 45sec recipe for 4" samples
- Load sample and check centering
- Dispense PMMA A4 using a pipette and click Start Process
- Once the spin is complete, transfer to hotplate at 180°C for 180 sec
Exposure
Exposure is performed on the JEOL E-Beam. Exposure dosage will depend on the materials on the sample and feature size. The standard exposure on silicon is 650 μC/cm2. For an oxide film, this can be increased to 675 μC/cm2. For large or varied features, the tool supports proximity correction.
For assistance characterizing exposure dose, please create a helpdesk ticket.
Development
PMMA is developed with MIBK in the E-Beam Solvent Bench.
- Develop sample in a 1:3 mixture of MIBK:IPA for 60 sec
- Rinse sample in IPA for 30 sec
- Blow the sample dry with a N2 gun