l_nit350 is a higher temp nitride deposition recipe for the Plasmatherm 790. It is optimized to have a stress near 25 MPa and an index of 2.0.
About this Process | |
---|---|
Process Details | |
Equipment | Plasmatherm 790 |
Technology | PECVD |
Material | Si3N4 |
Gases Used | SiH4, NH3, N2 |
Parameters
Parameter | Dep |
---|---|
RF Power | 150 W |
Pressure | 1500 mTorr |
NH3 Flow | 1.43 sccm |
N2 Flow | 160 sccm |
He Flow | 490 sccm |
SiH4 Flow | 5 sccm |
Temperature | 350°C |
Capabilities
Parameter | |
---|---|
Deposition Rate | 4.3 Å/sec |
Index of Refraction | 2.00 ± 0.02 |
Stress | 50 ± 50 MPa |
This recipe has also show to work as a KOH mask.
Qualification
Occasionally L_nit350 is tested on a 100 mm Si wafer. The results can be seen below.