Occasionally L_nit350 is tested on a 100 mm Si wafer.  The results can be seen below.
 
Occasionally L_nit350 is tested on a 100 mm Si wafer.  The results can be seen below.
 +
 +
{{expand section|need the chart}}

Revision as of 14:45, 29 July 2015

l_nit350 is a higher temp nitride deposition recipe for the Plasmatherm 790. It is optimized to have a stress near 25 MPa and an index of 2.0.

About this Process
Process Details
Equipment Plasmatherm 790
Technology PECVD
Material Si3N4
Gases Used SiH4, NH3, N2



Parameters

Parameter Dep
RF Power 150 W
Pressure 1500 mTorr
NH3 Flow 1.43 sccm
N2 Flow 160 sccm
He Flow 490 sccm
SiH4 Flow 5 sccm
Temperature 350°C

Capabilities

Parameter
Deposition Rate 4.3 Å/sec
Index of Refraction 2.00 ± 0.02
Stress 50 ± 50 MPa

This recipe has also show to work as a KOH mask.

Qualification

Occasionally L_nit350 is tested on a 100 mm Si wafer. The results can be seen below.