Plasmatherm 790/Processes/L nit350
< Plasmatherm 790 | Processes
Jump to navigation
Jump to search
Revision as of 08:55, 28 July 2015 by Wrightsh (talk | contribs) (Created page with "m_nit350 is a higher temp nitride deposition recipe for the Plasmatherm 790 Category:Processes {{Infobox process |image = |caption = |technology = PECVD |mate...")
m_nit350 is a higher temp nitride deposition recipe for the Plasmatherm 790
About this Process | |
---|---|
Process Details | |
Equipment | Plasmatherm 790 |
Technology | PECVD |
Material | Si3N4 |
Gases Used | SiH4, NH3, N2 |
Parameters
Parameter | Dep |
---|---|
RF Power | 100 W |
Pressure | 2000 mTorr |
NH3 Flow | 1.8 sccm |
N2 Flow | 1500 sccm |
SiH4 Flow | 5 sccm |
Temperature | 350°C |
Capabilities
Parameter | |
---|---|
Deposition Rate | 5.9 Å/sec |
Index of Refraction | 2.02 |
Stress | 519 MPa |
Roughness | ? |
Limitations
The limitations for this recipe are still being defined.
Qualification
Occasionally m_nit350 is tested on a 100 mm Si wafer. The deposition rate can be seen below for m_nit200, 260 and 350.