Open main menu

Plasmatherm 790/Processes/L ox350

< Plasmatherm 790‎ | Processes
Revision as of 10:36, 28 October 2021 by Wrightsh (talk | contribs) (→‎Capabilities)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

l_ox350 is a higher temp oxide deposition recipe for the Plasmatherm 790.

About this Process
Process Details
Equipment Plasmatherm 790
Technology PECVD
Material SiO2
Gases Used SiH4, N2O, He



Capabilities

Parameter
Deposition Rate 44.5 nm/min
Index of Refraction 1.467
Stress -420 MPa

Qualification is done with a 5 minute run, max allowed thickness of 2µm.

Parameters

Parameter Dep
RF Power 75 W
Pressure 900 mTorr
SiH4 Flow 3.0 sccm
N2O Flow 200 sccm
He Flow 100 sccm
Temperature 350°C