Plasmatherm 790/Processes/L ox350

From LNF Wiki
< Plasmatherm 790‎ | Processes
Revision as of 12:10, 15 January 2025 by Mcmyles (talk | contribs) (→‎Capabilities)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Jump to navigation Jump to search

l_ox350 is a higher temp oxide deposition recipe for the Plasmatherm 790.

About this Process
Process Details
Equipment Plasmatherm 790
Technology PECVD
Material SiO2
Gases Used SiH4, N2O, He



Capabilities

Parameter
Deposition Rate 44.5 nm/min
Index of Refraction 1.467
Stress -420 MPa

Qualification is done with a 5 minute run, max allowed thickness of 2µm. Once you have deposited 2um of oxide, you must run a clean process to "reset" the chamber.

Parameters

Parameter Dep
RF Power 75 W
Pressure 900 mTorr
SiH4 Flow 3.0 sccm
N2O Flow 200 sccm
He Flow 100 sccm
Temperature 350°C