Difference between revisions of "Plasmatherm 790/Processes/L ox350R"

From LNF Wiki
Jump to navigation Jump to search
Line 57: Line 57:
 
|-
 
|-
 
|}
 
|}
 +
 +
Qualification is done with a 5 minute run, max allowed thickness of 2µm.

Revision as of 15:39, 26 March 2018

L_OX350R is a 350 C oxide deposition recipe designed to reduce the film roughness by increasing the power. Currently more characterization is needed but roughness as low as 0.23 nm have been seen.

About this Process
Process Details
Equipment Plasmatherm 790
Technology PECVD
Material SiO2
Gases Used SiH4, N2O, He



Parameters

Parameter Dep
RF Power 150 W
Pressure 900 mTorr
SiH4 Flow 3.0 sccm
N2O Flow 200 sccm
He Flow 100 sccm
Temperature 350°C

Capabilities

Parameter
Deposition Rate 6.5 Å/sec
Index of Refraction ?
Stress ? MPa

Qualification is done with a 5 minute run, max allowed thickness of 2µm.