m_pary1 is an O2 etch that can be used for parylene and other polymers.

About this Process
Process Details
Equipment Plasmatherm 790
Technology RIE
Material Parylene
Mask Materials Photoresist
Gases Used O2



Parameters

Parameter Etch
RF Power 105 W
Pressure 100 mTorr
O2 Flow 99 sccm

Capabilities

Etch Rate

Mask Selectivity

  • Si Etch Rate: <5 Å/min
  • SiO2 Etch Rate: <5 Å/min

Sidewall Profile

  • Undercut: ?

Limitations