SPR 220 is our most commonly used photoresist, especially for RIE. The lab stocks SPR 220 (3.0) for general use, in the ACS 200 Cluster Tool, and in the CEE 200X #1 & #2. For films thicker then 5µm SPR 220 (7.0) is also available from the LNF Store.
Contents
3µm - SPR 220 (3.0)
Process
- Dehydrate and apply HMDS
- Spin
- Bake 115°C for 90 sec
- Wait ≥5 min
- Expose
- Stepper
- Silicon - 0.40 sec
- Aluminum (~90% reflection) - 0.34 sec
- ~15% reflection - 0.42 sec
- Aligner - 7 sec (silicon)
- Stepper
- Wait ≥3 min
- Bake 115°C for 90 sec
- Develop
- ACS - AZ300 - 30 sec
- CEE - AZ726 30-30 DP
Characterization
Stepper
Minimum Feature Size | |
---|---|
Grating | 700 nm |
Line | ?? |
Trench | 1 µm |
Hole | ?? |
Pillar | ?? nm |
Gratings with equal duty cycle.
Free standing trenches.
Free standing lines.
- TODO
Holes
- TODO
Pillars
- TODO
Focus should be kept at 0.
Puddle vs Spray Develop
- TODO
Contact Aligner
~2µm minimum feature size, but this is partially limited by the mask maker.
5µm of SPR 220 (3.0)
10µm - SPR 220 (7.0)
Process
- Dehydrate and apply HMDS
- Spin on ACS at 2000 RPM or on CEE 200X PR Spinners at 2000 RPM
- Bake 6 minutes (360 seconds) at 115°C
- Wait ≥ 20 min
- Expose
- Stepper
- Silicon - ??
- Aluminum (~90% reflection) - ??
- ~15% reflection - ??
- Aligner -?? sec (silicon)
- Stepper
- Wait ≥60 min
- Bake 115°C for 90 sec
- Develop
- ACS - AZ300 - 60 sec
- CEE - AZ726 60-60 DP