Difference between revisions of "SPR 220 7.0"

From LNF Wiki
Jump to navigation Jump to search
Line 43: Line 43:
 
===Bubbles in resist after spinning===
 
===Bubbles in resist after spinning===
 
===Cracking Resist===
 
===Cracking Resist===
 +
This has been traced back to how you cool your sample. Best results have been seen with the following options.
 +
*Place sample in a 25 wafer carrier well away from the table and let sit for 2-3 minutes (this is what is used for the characterization work)
 +
* These are options that other cleanroom users use. They may affect other aspect ration and exposure conditions.
 +
**Step down to a 90°C hotplate for 30 seconds after 115°C step and then place on a wipe folded in quarters.
 +
**Step down to a 90°C hotplate for 60 seconds, step down to a 65°C hotplate for 60 sec, cool on a stack of wipes.
 +
 
===Small bubbles form during DRIE===
 
===Small bubbles form during DRIE===
 
===Resist peeling during DRIE===
 
===Resist peeling during DRIE===

Revision as of 14:16, 24 March 2020

SPR 220 is our most commonly used photoresist, especially for RIE. The lab stocks SPR 220 (3.0) for general use, in the ACS 200 cluster tool, and in the CEE 200X photoresist spinner 2. For films thicker then 5µm SPR 220 (7.0) is also available from the LNF Store and in the CEE 200X photoresist spinner 1.

Process

  1. Dehydrate and apply HMDS
  2. CEE 200X photoresist spinner 1, 10um recipe
  3. Soft bake
    • Use 2 Hotplates - 30 seconds @ 90°C, 6 minutes (360 seconds) at 115°C. Move quickly between hotplates to wafer does not cool.
    • Let sample cool in a cassette or somewhere it can cool slowly. NOT on cold metal table.
  4. Wait ≥ 20 min
  5. Expose
    • MA/BA 6 - Aligner -26 sec (silicon)
  6. Wait ≥60 min
  7. Bake 115°C for
    • Use 2 Hotplates - 30 seconds @ 90°C, 3 minutes (180 seconds) at 115°C. Move quickly between hotplates to wafer does not cool.
    • Let sample cool in a cassette or somewhere it can cool slowly. NOT on cold metal table.
  8. Develop
    • ACS - AZ300 - ?? sec
    • CEE - AZ726 DP 80-80 sec

Characterization

Softbake

Wait time after Softbake

Exposure

Wait time between Exposure and Post Exposure Bake

Waittime.jpg

There are still some bubbles after 50 minutes so wait time needs to be greater than 50 minutes.

Post Exposure Bake

PEB matrix2.jpg

Develop

Developer Matrix, 4um.jpg

Troubleshooting

Bubbles in resist after spinning

Cracking Resist

This has been traced back to how you cool your sample. Best results have been seen with the following options.

  • Place sample in a 25 wafer carrier well away from the table and let sit for 2-3 minutes (this is what is used for the characterization work)
  • These are options that other cleanroom users use. They may affect other aspect ration and exposure conditions.
    • Step down to a 90°C hotplate for 30 seconds after 115°C step and then place on a wipe folded in quarters.
    • Step down to a 90°C hotplate for 60 seconds, step down to a 65°C hotplate for 60 sec, cool on a stack of wipes.

Small bubbles form during DRIE

Resist peeling during DRIE