Difference between revisions of "SPR 220 7.0"
m |
|||
Line 7: | Line 7: | ||
=Process= | =Process= | ||
# Dehydrate and apply HMDS | # Dehydrate and apply HMDS | ||
− | # [[CEE 200X photoresist spinner 1]], 10um recipe | + | # Spin |
+ | #* [[CEE 200X photoresist spinner 1]], 10um recipe | ||
+ | #* [[ACS 200 cluster tool]], 10um recipe with external syringe | ||
+ | #* [[CEE 100CB photoresist spinner]], manual syringe at ~____rpm | ||
# Soft bake | # Soft bake | ||
− | #*Use 2 Hotplates - 30 | + | #*Use 2 Hotplates - 90°C 30 sec → 115°C 6 min. Move quickly between hotplates so wafer does not cool. |
− | #* Let sample cool in a cassette or somewhere it can cool slowly | + | #* Let sample cool in a cassette or somewhere it can cool slowly, NOT on cold metal table. Cooling the wafer too quickly can cause the resist to crack. |
− | # Wait ≥ 20 min | + | # Wait ≥ 20 min (rehydration) |
# Expose | # Expose | ||
− | #* | + | #* Aligner - 26 sec (silicon) |
− | # Wait | + | # Wait ≥ 60 min (outgassing) |
− | # Bake | + | # Post Exposure Bake |
− | #*Use 2 Hotplates - 30 | + | #*Use 2 Hotplates - 90°C 30 sec → 115°C 3 min. Move quickly between hotplates to wafer does not cool. |
− | #*Let sample cool in a cassette or somewhere it can cool slowly | + | #* Let sample cool in a cassette or somewhere it can cool slowly, NOT on cold metal table. Cooling the wafer too quickly can cause the resist to crack. |
# Develop | # Develop | ||
#* ACS - AZ300 - ?? sec | #* ACS - AZ300 - ?? sec |
Revision as of 09:42, 25 March 2020
This page is currently being expanded. |
SPR 220 is our most commonly used photoresist, especially for RIE. The lab stocks SPR 220 (3.0) for general use, in the ACS 200 cluster tool, and in the CEE 200X photoresist spinner 1 & CEE 200X photoresist spinner 2. For films thicker then 5µm SPR 220 (7.0) is also available from the LNF Store and in the CEE 200X photoresist spinner 1.
Contents
Process
- Dehydrate and apply HMDS
- Spin
- CEE 200X photoresist spinner 1, 10um recipe
- ACS 200 cluster tool, 10um recipe with external syringe
- CEE 100CB photoresist spinner, manual syringe at ~____rpm
- Soft bake
- Use 2 Hotplates - 90°C 30 sec → 115°C 6 min. Move quickly between hotplates so wafer does not cool.
- Let sample cool in a cassette or somewhere it can cool slowly, NOT on cold metal table. Cooling the wafer too quickly can cause the resist to crack.
- Wait ≥ 20 min (rehydration)
- Expose
- Aligner - 26 sec (silicon)
- Wait ≥ 60 min (outgassing)
- Post Exposure Bake
- Use 2 Hotplates - 90°C 30 sec → 115°C 3 min. Move quickly between hotplates to wafer does not cool.
- Let sample cool in a cassette or somewhere it can cool slowly, NOT on cold metal table. Cooling the wafer too quickly can cause the resist to crack.
- Develop
- ACS - AZ300 - ?? sec
- CEE - AZ726 DP 80-80 sec
Characterization
Softbake
Wait time after Softbake
Exposure
Wait time between Exposure and Post Exposure Bake
There are still some bubbles after 50 minutes so wait time needs to be greater than 50 minutes.
Post Exposure Bake
Develop
Troubleshooting
Bubbles in resist after spinning
Cracking Resist
This has been traced back to how you cool your sample. Best results have been seen with the following options.
- Place sample in a 25 wafer carrier well away from the table and let sit for 2-3 minutes (this is what is used for the characterization work)
- These are options that other cleanroom users use. They may affect other aspect ration and exposure conditions.
- Step down to a 90°C hotplate for 30 seconds after 115°C step and then place on a wipe folded in quarters.
- Step down to a 90°C hotplate for 60 seconds, step down to a 65°C hotplate for 60 sec, cool on a stack of wipes.
Small bubbles form during DRIE
This could be potentially be caused by UV exposure and simultaneous heating during the DRIE step creating N2 bubble. After develop
- Flood Expose Sample for 45 sec on MA/BA6
- Wait >1hr
- DRIE
Resist peeling during DRIE
This is has been tracked back to cooling after mounting your sample for DRIE.
- After mounting sample remove from hotplate.
- Let cool for at least 5 minutes.