Difference between revisions of "SPR 955"

From LNF Wiki
Jump to navigation Jump to search
Line 2: Line 2:
 
{{#ifeq: {{NAMESPACE}} | Template | | [[Category:Chemicals]]}}
 
{{#ifeq: {{NAMESPACE}} | Template | | [[Category:Chemicals]]}}
  
SPR 955 is an I-line series of photoresists developed by ''microchem'', it's similar to SPR 220 but is formulated for thinner viscosities and higher resolution.  We've been able to consistently get 500nm gratings in 0.97µm of SPR 955 in the stepper, on silicon.  The 0.97µm thickness was chosen because it's one of the peaks listed in the datasheets swing curve.
+
SPR 955 is an I-line series of photoresists developed by ''microchem'', it's similar to SPR 220 but is formulated for thinner viscosities and higher resolution.  We've been able to consistently get 500nm gratings in 0.97µm of SPR 955 in the stepper, on silicon.  The 0.97µm thickness was chosen because it's one of the peaks listed in the datasheets swing curve.  At this thickness substrates with moderate to high reflection of 365nm light will be more sensitive to the exposure time / actual thickness of the resist.
  
==Processes==
+
==SPR 955 (0.97µm)==
===SPR 955 (0.97µm)===
+
===Process===
 
# Vapor prime wafer with HMDS
 
# Vapor prime wafer with HMDS
 
# Spin 0.97µm in ACS, CEE 200X #1 or CEE 100CB
 
# Spin 0.97µm in ACS, CEE 200X #1 or CEE 100CB
Line 41: Line 41:
 
Notes: When photoresist is this thin the swing curve will have a larger effect; small thickness variations will have a larger change in the necessary exposure.  Also at the end of the process you will have closer to .9-.94µm of resist.  The softbake needs to be at 100C, not 115.  Doing the softbake at 115 will burn out a lot of the PAC's, increasing dose to clear by ~40% (.24 sec vs .17 sec on the stepper).
 
Notes: When photoresist is this thin the swing curve will have a larger effect; small thickness variations will have a larger change in the necessary exposure.  Also at the end of the process you will have closer to .9-.94µm of resist.  The softbake needs to be at 100C, not 115.  Doing the softbake at 115 will burn out a lot of the PAC's, increasing dose to clear by ~40% (.24 sec vs .17 sec on the stepper).
  
 +
 +
===Silicon===
 
These gratings are on silicon and exposed via the stepper:
 
These gratings are on silicon and exposed via the stepper:
 
 
[[File:SPR_955_2um_grating.png|borderless|600px]]
 
[[File:SPR_955_2um_grating.png|borderless|600px]]
 
[[File:SPR_955_500nm_grating.jpg|borderless|600px]]
 
[[File:SPR_955_500nm_grating.jpg|borderless|600px]]
 +
 +
===Low Reflection Substrate===
 +
====Gratings====
 +
====Isolated Lines====
 +
The minimum size of an isolated line in a stepper is really limited by how well the substrate is in focus since it's really two large features (that can pass many orders through the lens) next to each other. Especially below 500nm you start to get pretty strong CD loss.  And although 350nm & 400nm lines can typically be printed, small changes if how well the substrate is focused will have large changes in CD.
 +
====Isolated Trenches====
 +
Although you can get a nominal 350 / 400nm isolated trench to print, the physical size of it is going to end up closer to 500nm, as shown below.
 +
  
 
==Process Curves==
 
==Process Curves==

Revision as of 20:08, 11 September 2019


SPR 955 is an I-line series of photoresists developed by microchem, it's similar to SPR 220 but is formulated for thinner viscosities and higher resolution. We've been able to consistently get 500nm gratings in 0.97µm of SPR 955 in the stepper, on silicon. The 0.97µm thickness was chosen because it's one of the peaks listed in the datasheets swing curve. At this thickness substrates with moderate to high reflection of 365nm light will be more sensitive to the exposure time / actual thickness of the resist.

SPR 955 (0.97µm)

Process

  1. Vapor prime wafer with HMDS
  2. Spin 0.97µm in ACS, CEE 200X #1 or CEE 100CB
  3. Bake at 100°C for 90 sec
  4. Verify thickness if possible, for thin resists small thickness variations drastically change the necessary exposure dose.
  5. Expose
Material Stepper Contact Aligner Notes
Silicon 0.30 sec 5.5 sec
500nm SiO2
Borosilicate 0.30-0.34 Severe sidewall degradation <1µm due to back reflection
  1. Bake at 110°C for 90 sec
  2. Develop

Notes: When photoresist is this thin the swing curve will have a larger effect; small thickness variations will have a larger change in the necessary exposure. Also at the end of the process you will have closer to .9-.94µm of resist. The softbake needs to be at 100C, not 115. Doing the softbake at 115 will burn out a lot of the PAC's, increasing dose to clear by ~40% (.24 sec vs .17 sec on the stepper).


Silicon

These gratings are on silicon and exposed via the stepper: borderless borderless

Low Reflection Substrate

Gratings

Isolated Lines

The minimum size of an isolated line in a stepper is really limited by how well the substrate is in focus since it's really two large features (that can pass many orders through the lens) next to each other. Especially below 500nm you start to get pretty strong CD loss. And although 350nm & 400nm lines can typically be printed, small changes if how well the substrate is focused will have large changes in CD.

Isolated Trenches

Although you can get a nominal 350 / 400nm isolated trench to print, the physical size of it is going to end up closer to 500nm, as shown below.


Process Curves

This plot shows the ideal exposure time for several develops in the ACS. The 0.3 sec exposure with a AZ 300 25 sec develop in the ACS seems to be a good point.

SPR 955 0.97µm CD Loss vs Exposure.png

The next plot shows the CD loss vs the amount of defocus in the stepper. ±900nm is about the limit before it's no longer going to work. Larger features will of course have a wider focus range.

Stepper 500nm Grating SPR 955 0.97µm CD Loss vs Defocus.png