Difference between revisions of "STS APS DGRIE/Processes/LNF Polymer"

From LNF Wiki
Jump to navigation Jump to search
(Created page with "<!-- Make sure to add any other relevant categories --> {{Infobox process |technology = RIE |material = Polyimide |mask = Photoresist, SiO<sub>2</sub>, Aluminum |gases = O<sub...")
 
 
(4 intermediate revisions by 2 users not shown)
Line 1: Line 1:
<!-- Make sure to add any other relevant categories -->
 
 
{{Infobox process
 
{{Infobox process
 
|technology = RIE
 
|technology = RIE
Line 8: Line 7:
 
|modified =   
 
|modified =   
 
|authors = Shawn Wright & Kevin Owen
 
|authors = Shawn Wright & Kevin Owen
}}
+
}} [[Category:Processes]] [[Category:RIE]]
[[Category:Processes]]  
 
[[Category:RIE]]
 
  
This is an O<sub>2</sub> etch for polymers like polyimide.
+
[[{{PAGENAME}}|{{SUBPAGENAME}}]] is an O<sub>2</sub> based plasma etch for thin film polymers (e.g. [[polyimide]], [[parylene]]).
 
 
 
 
==Etch Rates==
 
*Polyimide: 920 nm/min
 
*SPR 220: ?? nm/min
 
*Aluminum: ?? nm/min
 
*Platinum: ~1.5 nm/min
 
  
 +
==Procedure==
 +
Follow the instructions in the tool [[{{ROOTPAGENAME}}#Standard operating procedure|operating procedure]] and select ''LNF Polymer'' from the supported processes folder.
  
 
==Parameters==
 
==Parameters==
Line 31: Line 23:
 
|5 mTorr
 
|5 mTorr
 
|-
 
|-
|TCP Power
+
|ICP Power
 
|2000 W
 
|2000 W
 
|-
 
|-
Line 42: Line 34:
 
|He Flow
 
|He Flow
 
|100 sccm
 
|100 sccm
|-
+
|}
 +
 
 +
==Characterization==
 +
<!-- Use this section to put any characterization data. Examples in headings below. Can go in separate sections or a bulleted list.-->
 +
 
 +
===Etch Rate===
 +
*Polyimide: 920 nm/min
 +
*Parylene: 1.3 µm/min (user reported)
 +
 
 +
===Uniformity===
 +
Not tested.
 +
 
 +
===Mask selectivity===
 +
*Platinum: ~1.5 nm/min
 +
*SiO<sub>2</sub>: 28 nm/min
 +
*Aluminum: < 2 nm/min (varies with etch time; e.g. 30 sec or less is higher, ~4 nm/min) (user reported)
 +
 
 +
==Limitations==
 +
Oxygen plasmas are predominantly isotropic; the specific isotropy ratio has not been measured for this process. Standard photoresist masks are not recommended, since they are polymers and will also etch quickly with this process. However, there are limitations to what type of hard mask is acceptable, so please create a helpdesk ticket to discuss your process with a tool engineer.
 +
 
 +
==Qualification==
 +
None at this time.

Latest revision as of 14:51, 30 March 2022

About this Process
Process Details
Equipment STS APS DGRIE
Technology RIE
Material Polyimide
Mask Materials Photoresist, SiO2, Aluminum
Gases Used O2, He
Date Created October 2020
Authored By Shawn Wright & Kevin Owen

LNF Polymer is an O2 based plasma etch for thin film polymers (e.g. polyimide, parylene).

Procedure

Follow the instructions in the tool operating procedure and select LNF Polymer from the supported processes folder.

Parameters

Parameter Main Etch
Pressure 5 mTorr
ICP Power 2000 W
Bias Power 30 W
O2 Flow 90 sccm
He Flow 100 sccm

Characterization

Etch Rate

  • Polyimide: 920 nm/min
  • Parylene: 1.3 µm/min (user reported)

Uniformity

Not tested.

Mask selectivity

  • Platinum: ~1.5 nm/min
  • SiO2: 28 nm/min
  • Aluminum: < 2 nm/min (varies with etch time; e.g. 30 sec or less is higher, ~4 nm/min) (user reported)

Limitations

Oxygen plasmas are predominantly isotropic; the specific isotropy ratio has not been measured for this process. Standard photoresist masks are not recommended, since they are polymers and will also etch quickly with this process. However, there are limitations to what type of hard mask is acceptable, so please create a helpdesk ticket to discuss your process with a tool engineer.

Qualification

None at this time.