Difference between revisions of "STS Pegasus 4/Processes/LNF Recipe 1"

From LNF Wiki
Jump to navigation Jump to search
 
(5 intermediate revisions by the same user not shown)
Line 1: Line 1:
{{copy edit}}
+
[[Category:Processes]]{{Infobox process
{{Infobox process
 
 
|image = STS Pegasus_4_Recipe_1_2_um.jpg
 
|image = STS Pegasus_4_Recipe_1_2_um.jpg
 
|caption = Recipe 1 for 20 min, 2 µm Trench
 
|caption = Recipe 1 for 20 min, 2 µm Trench
Line 11: Line 10:
 
|authors = SPTS, Brian Vanderelzen, Kevin Owen
 
|authors = SPTS, Brian Vanderelzen, Kevin Owen
 
}}
 
}}
Recipe 1 is the base silicon etch for the pegasus tools.  It has a high selectivity, moderately fast etch rate and a clean profile.
+
'''{{SUBPAGENAME}}''' is the base silicon etch for the pegasus tools.  It has a high selectivity, moderately fast etch rate and a clean profile.
  
 
==Procedure==
 
==Procedure==
Line 62: Line 61:
 
|-  
 
|-  
 
| Chuck Temperature
 
| Chuck Temperature
|colspan="2" | 20°C
+
|colspan="3" | 20°C
 
|}
 
|}
  
Line 103: Line 102:
 
===Etch Rate===
 
===Etch Rate===
 
The etch rate will vary with the size of the trench being etched.  Larger trenches tend to etch faster, this trend can be seen below.
 
The etch rate will vary with the size of the trench being etched.  Larger trenches tend to etch faster, this trend can be seen below.
 +
 
{{#widget:Iframe
 
{{#widget:Iframe
 
|url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=138105026&format=image     
 
|url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=138105026&format=image     
Line 116: Line 116:
 
===Mask Selectivity===
 
===Mask Selectivity===
 
* Photoresist Etch Rate
 
* Photoresist Etch Rate
** [[SPR 220]]: 840 Å/min  
+
** [[SPR 220]]: 500 Å/min  
 
* [[SiO2|SiO<sub>2</sub>]] Etch Rate
 
* [[SiO2|SiO<sub>2</sub>]] Etch Rate
 
** Thermal oxide/HTO: 166 Å/min
 
** Thermal oxide/HTO: 166 Å/min
 
** LTO: 178 Å/min
 
** LTO: 178 Å/min
 
** PECVD: unknown
 
** PECVD: unknown
 +
* [[Silicon nitride]] Etch Rate
 +
** LPCVD Nitride: 356 Å/min
 +
** LPCVD Low Stress Nitride: 291 Å/min
  
 
===Sidewall Profile===
 
===Sidewall Profile===
Line 151: Line 154:
 
====Trench====
 
====Trench====
 
Running recipe 1 for 20 minutes with 3 µm of [[SPR 220]] on a silicon wafer with our standard DRIE characterization mask can produce a profile like this.
 
Running recipe 1 for 20 minutes with 3 µm of [[SPR 220]] on a silicon wafer with our standard DRIE characterization mask can produce a profile like this.
<gallery mode="packed-hover"  heights="200px">
+
<gallery mode="packed-hover"  heights="180px">
 
File:STS Pegasus_4_Recipe_1_2_um.jpg|Recipe 1 for 20 min, 2 µm Trench
 
File:STS Pegasus_4_Recipe_1_2_um.jpg|Recipe 1 for 20 min, 2 µm Trench
 
File:STS Pegasus_4_Recipe_1_10_um.jpg|Recipe 1 for 20 min, 10 µm Trench
 
File:STS Pegasus_4_Recipe_1_10_um.jpg|Recipe 1 for 20 min, 10 µm Trench

Latest revision as of 10:35, 26 March 2021

About this Process
STS Pegasus 4 Recipe 1 2 um.jpg
Recipe 1 for 20 min, 2 µm Trench
Process Details
Equipment STS Pegasus 4
Technology DRIE
Material Si
Mask Materials PR, SiO2
Gases Used SF6, C4F8, O2
Date Created Jan 1, 2009
Authored By SPTS, Brian Vanderelzen, Kevin Owen


LNF Recipe 1 is the base silicon etch for the pegasus tools. It has a high selectivity, moderately fast etch rate and a clean profile.

Procedure

LNF recipe 1 has 2 main process (DRIE) steps. For recipes shorter than 20 minutes, set the first DRIE step to the desired length. For recipes longer than 20 minutes, set the first DRIE step to 20:00 and the second DRIE step to the remaining time.

Run LNF Recipe 1 for up to 20 minutes with the 1 minute automated clean recipe, longer etches should be run with the 3 minute automated clean recipe.

Parameters

Parameter Dep Etch
Boost Main
ICP Power 2000 W 2800 W
Bias Power 0 W 60 W
Bias Pulsing N/A 40 Hz - 80%
Pressure 24 mTorr 30 mTorr
C4F8 Flow 250 sccm 30-0 sccm (ramped)
SF6 Flow 0 sccm 390 sccm
O2 Flow 0 sccm 39 sccm
Time 2.0 s 2.6 s
Chuck Temperature 20°C

Capabilities

This process, as is true with all Bosch processes, varies depending on feature size and density, due to RIE lag. The below table contains typical results for 2 µm, 10 µm, and 100 µm trenches and the following sections expand on these results. It is strongly recommended that the process is tested with any new mask.

Parameter 2 µm Trench 10 µm Trench 100 µm Trench
Etch Rate 3 µm/min 4.5 µm/min 5.6 µm/min
Undercut 160 nm 200 nm 200 nm
Scallop height 370 nm 390 nm 370 nm
Scallop depth 70 nm 50 nm
Sidewall angle 89.6° 89.7°

Etch Rate

The etch rate will vary with the size of the trench being etched. Larger trenches tend to etch faster, this trend can be seen below.

Mask Selectivity

  • Photoresist Etch Rate
  • SiO2 Etch Rate
    • Thermal oxide/HTO: 166 Å/min
    • LTO: 178 Å/min
    • PECVD: unknown
  • Silicon nitride Etch Rate
    • LPCVD Nitride: 356 Å/min
    • LPCVD Low Stress Nitride: 291 Å/min

Sidewall Profile

Mask undercut, scalloping, and sidewall angle are shown below.

Trench

Running recipe 1 for 20 minutes with 3 µm of SPR 220 on a silicon wafer with our standard DRIE characterization mask can produce a profile like this.

Limitations

LNF Recipe 1 is known to work under a range of conditions. Outside of these conditions, etch performance is not guaranteed. Etch rates will vary depending on feature size, etch length, open area, etc. We strongly recommend testing the process prior to running device wafers.

One common problem seen when running outside of these conditions is grassing. This occurs when the C4F8/SF6 ratio is unbalanced causing micromasking. This creates tiny pillars of un-etched Si and teflon on the surface of the feature. An example of grassing can be seen below.

Grass (brown area) on perimeter of wafer

Etch Length

  • Generally 30 sec - 20 minutes is known to work well.
  • Recipe 1 is known to work well up to 20 min of etching. The process is tested for 20 min monthly to verify performance. Longer etches, particularly >30 min will likely cause undesirable results.
  • Etches longer than 20 minutes should use the second DRIE step for any time past 20 minutes. This removes the C4F8 from the etch step to help reduce grassing.

Feature Size

  • Tested on features from 1 μm - 100 μm.
  • The standard characterization pattern used to qualify Recipe 1 has open lines, trenches, and grating patterns from 1 μm - 100 μm. Larger and smaller features have not been tested and may not provide the expected results.

Aspect ratio

  • Aspect ratio limitations vary depending on feature size. For instance, 2 μm features have an aspect ratio limit of around 50:1. For larger features, aspect ratio is typically limited to etch length (see above).

Open area

  • Very large features and masks with total open area >20% are known to degrade etch performance and should be tested prior to running device wafers. For masks with more than 20% open area Recipe 3 may provide better results.

Multi-step etching

  • Multi-step processing (i.e. running two or more etches with overlapping features) with the Bosch process is known to cause undesirable results. Please contact the tool engineers if you wish to run such a process so we can help reduce or eliminate issues.

Qualification

Every third Friday Recipe 1 is run for 20 minutes on a Si wafer with our standard DRIE characterization mask, with 3 µm of SPR 220. This is performed after the weekly clean, and a 100 µm trench is measured in 5 locations with the Zygo NewView 5000. This etch rate is reported in the chart below.