Difference between revisions of "STS Pegasus 4/Processes/LNF Recipe 3"
(Created page with "<!-- Make sure to add any other relevant categories --> Category:Processes {{warning|This page has not been released yet.}} {{Infobox process |technology = RIE |material =...") |
|||
(16 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
<!-- Make sure to add any other relevant categories --> | <!-- Make sure to add any other relevant categories --> | ||
− | [[Category:Processes]] | + | [[Category:Processes]]{{Infobox process |
− | + | |technology = DRIE | |
− | {{Infobox process | + | |material = [[Silicon|Si]] |
− | |technology = | + | |mask = [[Photoresist|PR]], [[Silicon dioxide|SiO2]] |
− | |material = Si | + | |gases = [[SF6|SF<sub>6</sub>]], [[C4F8|C<sub>4</sub>F<sub>8</sub>]], [[O2|O<sub>2</sub>]] |
− | |mask = [[Photoresist|PR]], [[Silicon | ||
− | |gases = | ||
|created = Jan 1, 2011 | |created = Jan 1, 2011 | ||
|modified = | |modified = | ||
|authors = Kevin Owen | |authors = Kevin Owen | ||
}} | }} | ||
− | Recipe | + | '''{{SUBPAGENAME}}''' is designed for deep and through wafer etching particularly on masks with a large exposed area (>20%). Undercut and scalloping is larger than LNF Recipe 1, but etch rates are higher (4-16 μm/min). |
==Procedure== | ==Procedure== | ||
<!-- Insert the SOP on the process here --> | <!-- Insert the SOP on the process here --> | ||
− | Run LNF Recipe | + | Run LNF Recipe 3 for up to 20 minutes with the 1 minute automated clean recipe, longer etches should be run with the 3 minute automated clean recipe. |
==Recipe Parameters== | ==Recipe Parameters== | ||
− | {| class="wikitable" border="1" | + | {| class="wikitable" border="1" style="text-align: center" |
|- | |- | ||
− | ! Parameter | + | ! rowspan="2"|Parameter |
− | ! Dep | + | ! rowspan="2"|Dep |
− | ! Etch | + | ! colspan="2"|Etch |
+ | |- | ||
+ | ! Boost | ||
+ | ! Main | ||
|- | |- | ||
| ICP Power | | ICP Power | ||
− | | | + | | 2000 W |
− | | | + | |colspan="2"| 4000 W |
|- | |- | ||
| Bias Power | | Bias Power | ||
− | | | + | | 0 W |
− | | | + | | 100 W |
+ | | 50 W | ||
|- | |- | ||
| Bias Pulsing | | Bias Pulsing | ||
− | | | + | | N/A |
− | | | + | |colspan="2"| 40 Hz 80% |
|- | |- | ||
| Pressure | | Pressure | ||
− | | | + | | 25 mTorr |
− | | | + | | 30 mTorr |
+ | | 100 mTorr | ||
|- | |- | ||
− | | | + | | C<sub>4</sub>F<sub>8</sub> Flow |
− | | | + | | 200 sccm |
− | | | + | |colspan="2"| 0 sccm |
|- | |- | ||
− | | | + | | SF<sub>6</sub> Flow |
− | | | + | | 0 sccm |
− | | | + | |colspan="2"| 600 sccm |
|- | |- | ||
− | | | + | | O<sub>2</sub> Flow |
− | | | + | | 0 sccm |
− | | | + | |colspan="2"| 60 sccm |
|- | |- | ||
| Time | | Time | ||
− | | | + | | 4 s |
− | | | + | | 2 s |
+ | | 6.5 s | ||
+ | |- | ||
+ | | Chuck Temperature | ||
+ | |colspan="3" | 10°C | ||
+ | |} | ||
+ | |||
+ | ==Capabilities== | ||
+ | This process, as is true with all Bosch processes, varies depending on feature size and density, due to [[:Category:DRIE#Aspect ratio dependent etching|RIE lag]]. The below table contains typical results for 2 µm, 10 µm, and 100 µm trenches and the following sections expand on these results. It is strongly recommended that the process is tested with any new mask. | ||
+ | |||
+ | {| class="wikitable" border="1" style="text-align: center" | ||
+ | |- | ||
+ | ! Parameter | ||
+ | ! 2 µm Trench | ||
+ | ! 10 µm Trench | ||
+ | ! 100 µm Trench | ||
+ | |- | ||
+ | | Etch Rate | ||
+ | | 7 µm/min | ||
+ | | 10.5 µm/min | ||
+ | | 15.8 µm/min | ||
+ | |- | ||
+ | | Undercut | ||
+ | | 0.83 µm | ||
+ | | 1.13 µm | ||
+ | | 1.13 µm | ||
+ | |- | ||
+ | | Scallop height | ||
+ | | 1.8 µm | ||
+ | | 2.5 µm | ||
+ | | 2.9 µm | ||
+ | |- | ||
+ | | Scallop depth | ||
+ | | 0.5 µm | ||
+ | | 0.7 µm | ||
+ | | 0.8 µm | ||
+ | |- | ||
+ | | Sidewall angle | ||
+ | | 90.1° | ||
+ | | 90.1° | ||
+ | | 90.2° | ||
|} | |} | ||
− | |||
===Etch Rate=== | ===Etch Rate=== | ||
The etch rate will vary with the size of the trench being etched. Larger trenches tend to etch faster, this trend can be seen below. | The etch rate will vary with the size of the trench being etched. Larger trenches tend to etch faster, this trend can be seen below. | ||
− | + | ||
− | + | {{#widget:Iframe | |
− | + | |url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=1796971608&format=image | |
+ | |width= 503.5 | ||
+ | |height= 311.3308333333333 | ||
+ | |border= 0 | ||
+ | |scrolling= no | ||
+ | }} | ||
===Mask Selectivity=== | ===Mask Selectivity=== | ||
* Photoresist Etch Rate | * Photoresist Etch Rate | ||
− | ** [[SPR 220]]: | + | ** [[SPR 220]]: 770 Å/min |
− | * [[ | + | * [[SiO2|SiO<sub>2</sub>]] Etch Rate |
− | ** Thermal oxide/HTO: | + | ** Thermal oxide: 222 Å/min |
− | ** LTO: | + | ** HTO: 219 Å/min |
+ | ** LTO: 230 Å/min | ||
** PECVD: unknown | ** PECVD: unknown | ||
+ | * [[Silicon nitride]] Etch Rate | ||
+ | ** LPCVD Nitride: 321 Å/min | ||
+ | ** LPCVD Low Stress Nitride: 223 Å/min | ||
+ | |||
+ | ===Sidewall Profile=== | ||
+ | Mask undercut, scalloping, and sidewall angle are shown below. | ||
+ | |||
+ | {{#widget:Iframe | ||
+ | |url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=992129259&format=image | ||
+ | |width= 503.5 | ||
+ | |height= 311.3308333333333 | ||
+ | |border= 0 | ||
+ | |scrolling= no | ||
+ | }} | ||
+ | |||
+ | {{#widget:Iframe | ||
+ | |url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=76533524&format=image | ||
+ | |width= 503.5 | ||
+ | |height= 311.3308333333333 | ||
+ | |border= 0 | ||
+ | |scrolling= no | ||
+ | }} | ||
+ | |||
+ | {{#widget:Iframe | ||
+ | |url= https://docs.google.com/spreadsheets/d/193-swCgAFeAuUAq5m6ewOFA-0r8uqdhZmkqVTSbZDwk/pubchart?oid=1310380588&format=image | ||
+ | |width= 503.5 | ||
+ | |height= 311.3308333333333 | ||
+ | |border= 0 | ||
+ | |scrolling= no | ||
+ | }} | ||
− | |||
====Trench==== | ====Trench==== | ||
− | Running recipe | + | Running recipe 3 for 20 minutes with 3 µm of [[SPR 220]] on a silicon wafer with our standard DRIE characterization mask can produce a profile like this. |
− | <gallery mode="packed-hover" heights=" | + | <gallery mode="packed-hover" heights="180px"> |
− | File:STS | + | File:STS Pegasus_4_Recipe_3_2_um.jpg|Recipe 3 for 20 min, 2 µm Trench |
− | File:STS | + | File:STS Pegasus_4_Recipe_3_10_um.jpg|Recipe 3 for 20 min, 10 µm Trench |
− | File:STS | + | File:STS Pegasus_4_Recipe_3_100_um.jpg|Recipe 3 for 20 min, 100 µm Trench |
</gallery> | </gallery> | ||
− | ==== | + | ==Limitations== |
− | An example of grassing can be seen below. | + | LNF Recipe 3 is known to work under a range of conditions. Outside of these conditions, etch performance is not guaranteed. Etch rates will vary depending on feature size, etch length, open area, etc. We strongly recommend testing the process prior to running device wafers. |
− | + | ||
− | File: | + | <!--One common problem seen when running outside of these conditions is [[Grass|grassing]]. This occurs when the C4F8/SF6 ratio is unbalanced causing micromasking. This creates tiny pillars of un-etched Si and teflon on the surface of the feature. An example of grassing can be seen below. |
− | + | ||
− | + | [[File:STS_Pegasus_4_Recipe_1_grass.jpg|Height:200px| Grass (brown area) on perimeter of wafer|thumbnail]]--> | |
− | |||
===Etch Length=== | ===Etch Length=== | ||
+ | *Generally 30 sec - 30 minutes is known to work well. | ||
+ | *Recipe 3 is tested for 10 min monthly to verify performance. | ||
+ | *Etches longer than 35 min are not well tested, since this is typically deeper than a standard thickness wafer. | ||
===Feature Size=== | ===Feature Size=== | ||
+ | *This recipe is designed for large (>10 μm) features. | ||
+ | *Smaller features often exhibit re-entrant (widening) sidewalls. | ||
+ | *The standard characterization pattern used to qualify Recipe 1 has open lines, trenches, and grating patterns from 1 μm - 100 μm. | ||
===Aspect ratio=== | ===Aspect ratio=== | ||
+ | *Aspect ratio limitations vary depending on feature size. For instance, 2 μm features have an aspect ratio limit of around 50:1. For larger features, aspect ratio is typically limited to the thickness of the wafer. | ||
===Open area=== | ===Open area=== | ||
+ | *This recipe will not produce grass up to 100% open area | ||
+ | *Large open areas (>50%) may require an SiO<sub>2</sub> mask, as excessive heating can cause photoresist to reticulate. | ||
+ | *Small (<20%) open area may cause an undesirable increase in etch rate or shift in sidewall profile due to excess Fluorine. | ||
===Multi-step etching=== | ===Multi-step etching=== | ||
Line 102: | Line 188: | ||
==Qualification== | ==Qualification== | ||
<!-- Insert a description of how the process is qualified, generally this should include a chart to show the processes stability over time--> | <!-- Insert a description of how the process is qualified, generally this should include a chart to show the processes stability over time--> | ||
− | Every third Friday Recipe | + | Every third Friday Recipe 3 is run for 10 minutes on a Si wafer with our standard DRIE characterization mask, with 3 µm of [[SPR 220]]. This is performed after the weekly clean, and a 100 µm trench is measured in 5 locations with the [[Zygo NewView 5000]]. This etch rate is reported in the chart below. |
{{#widget:Iframe | {{#widget:Iframe |
Latest revision as of 10:43, 26 March 2021
About this Process | |
---|---|
Process Details | |
Equipment | STS Pegasus 4 |
Technology | DRIE |
Material | Si |
Mask Materials | PR, SiO2 |
Gases Used | SF6, C4F8, O2 |
Date Created | Jan 1, 2011 |
Authored By | Kevin Owen |
LNF Recipe 3 is designed for deep and through wafer etching particularly on masks with a large exposed area (>20%). Undercut and scalloping is larger than LNF Recipe 1, but etch rates are higher (4-16 μm/min).
Contents
Procedure
Run LNF Recipe 3 for up to 20 minutes with the 1 minute automated clean recipe, longer etches should be run with the 3 minute automated clean recipe.
Recipe Parameters
Parameter | Dep | Etch | |
---|---|---|---|
Boost | Main | ||
ICP Power | 2000 W | 4000 W | |
Bias Power | 0 W | 100 W | 50 W |
Bias Pulsing | N/A | 40 Hz 80% | |
Pressure | 25 mTorr | 30 mTorr | 100 mTorr |
C4F8 Flow | 200 sccm | 0 sccm | |
SF6 Flow | 0 sccm | 600 sccm | |
O2 Flow | 0 sccm | 60 sccm | |
Time | 4 s | 2 s | 6.5 s |
Chuck Temperature | 10°C |
Capabilities
This process, as is true with all Bosch processes, varies depending on feature size and density, due to RIE lag. The below table contains typical results for 2 µm, 10 µm, and 100 µm trenches and the following sections expand on these results. It is strongly recommended that the process is tested with any new mask.
Parameter | 2 µm Trench | 10 µm Trench | 100 µm Trench |
---|---|---|---|
Etch Rate | 7 µm/min | 10.5 µm/min | 15.8 µm/min |
Undercut | 0.83 µm | 1.13 µm | 1.13 µm |
Scallop height | 1.8 µm | 2.5 µm | 2.9 µm |
Scallop depth | 0.5 µm | 0.7 µm | 0.8 µm |
Sidewall angle | 90.1° | 90.1° | 90.2° |
Etch Rate
The etch rate will vary with the size of the trench being etched. Larger trenches tend to etch faster, this trend can be seen below.
Mask Selectivity
- Photoresist Etch Rate
- SPR 220: 770 Å/min
- SiO2 Etch Rate
- Thermal oxide: 222 Å/min
- HTO: 219 Å/min
- LTO: 230 Å/min
- PECVD: unknown
- Silicon nitride Etch Rate
- LPCVD Nitride: 321 Å/min
- LPCVD Low Stress Nitride: 223 Å/min
Sidewall Profile
Mask undercut, scalloping, and sidewall angle are shown below.
Trench
Running recipe 3 for 20 minutes with 3 µm of SPR 220 on a silicon wafer with our standard DRIE characterization mask can produce a profile like this.
Limitations
LNF Recipe 3 is known to work under a range of conditions. Outside of these conditions, etch performance is not guaranteed. Etch rates will vary depending on feature size, etch length, open area, etc. We strongly recommend testing the process prior to running device wafers.
Etch Length
- Generally 30 sec - 30 minutes is known to work well.
- Recipe 3 is tested for 10 min monthly to verify performance.
- Etches longer than 35 min are not well tested, since this is typically deeper than a standard thickness wafer.
Feature Size
- This recipe is designed for large (>10 μm) features.
- Smaller features often exhibit re-entrant (widening) sidewalls.
- The standard characterization pattern used to qualify Recipe 1 has open lines, trenches, and grating patterns from 1 μm - 100 μm.
Aspect ratio
- Aspect ratio limitations vary depending on feature size. For instance, 2 μm features have an aspect ratio limit of around 50:1. For larger features, aspect ratio is typically limited to the thickness of the wafer.
Open area
- This recipe will not produce grass up to 100% open area
- Large open areas (>50%) may require an SiO2 mask, as excessive heating can cause photoresist to reticulate.
- Small (<20%) open area may cause an undesirable increase in etch rate or shift in sidewall profile due to excess Fluorine.
Multi-step etching
- Multi-step processing (i.e. running two or more etches with overlapping features) with the Bosch process is known to cause undesirable results. Please contact the tool engineers if you wish to run such a process so we can help reduce or eliminate issues.
Qualification
Every third Friday Recipe 3 is run for 10 minutes on a Si wafer with our standard DRIE characterization mask, with 3 µm of SPR 220. This is performed after the weekly clean, and a 100 µm trench is measured in 5 locations with the Zygo NewView 5000. This etch rate is reported in the chart below.