==Recipe Parameters==
 
==Recipe Parameters==
{| class="wikitable" border="1"
+
{| class="wikitable" border="1" style="text-align: center"
 
|-
 
|-
! Parameter
+
! rowspan="2"|Parameter
! Dep
+
! rowspan="2"|Dep
! Etch
+
! colspan="2"|Etch
 +
|-
 +
! Boost
 +
! Main
 
|-
 
|-
 
| ICP Power
 
| ICP Power
| W
+
| 2000 W
| W
+
|colspan="2"| 2500 W
 
|-
 
|-
 
| Bias Power
 
| Bias Power
| W
+
| 0 W
| W
+
| 80-100 W
 +
| 30 W
 
|-
 
|-
 
| Bias Pulsing
 
| Bias Pulsing
|  
+
| N/A
|  
+
|colspan="2"| 40 Hz - 80%
 
|-
 
|-
 
| Pressure
 
| Pressure
| mTorr
+
| 25 mTorr
| mTorr
+
|colspan="2"| 30 mTorr
 
|-
 
|-
| C4F8 Flow
+
| C<sub>4</sub>F<sub>8</sub> Flow
| sccm
+
| 90-140 sccm
| sccm
+
|colspan="2"| 0 sccm
 
|-
 
|-
| SF6 Flow
+
| SF<sub>6</sub> Flow
| sccm
+
| 0 sccm
| sccm
+
|colspan="2"| 110 sccm
 
|-
 
|-
| O2 Flow
+
| O<sub>2</sub> Flow
| sccm
+
| 0 sccm
| sccm
+
|colspan="2"| 10 sccm
 
|-
 
|-
 
| Time
 
| Time
| s
+
| 2.5 s
| s
+
| 3 s
 +
| 4 s
 +
|-
 +
| Temperature
 +
|colspan="3"| 10 C
 
|}
 
|}
  

Revision as of 11:17, 13 April 2018

Warning Warning: This page has not been released yet.
About this Process
Process Details
Equipment STS Pegasus 4
Technology DRIE
Material Si
Mask Materials PR, SiO2
Gases Used SF6, C4F8, O2
Date Created Jan 1, 2011
Authored By Kevin Owen


This highly specialized recipe is designed for high aspect ratio etching of small features (1-10 μm) with very low open area (<10%). The etch produces the most vertical sidewall with the least undercut, particularly at the top of the trench.

Procedure

Run LNF Recipe 4 for up to 20 minutes with the 1 minute automated clean recipe, longer etches should be run with the 3 minute automated clean recipe.

Recipe Parameters

Parameter Dep Etch
Boost Main
ICP Power 2000 W 2500 W
Bias Power 0 W 80-100 W 30 W
Bias Pulsing N/A 40 Hz - 80%
Pressure 25 mTorr 30 mTorr
C4F8 Flow 90-140 sccm 0 sccm
SF6 Flow 0 sccm 110 sccm
O2 Flow 0 sccm 10 sccm
Time 2.5 s 3 s 4 s
Temperature 10 C

Characterization

Etch Rate

The etch rate will vary with the size of the trench being etched. Larger trenches tend to etch faster, this trend can be seen below.

Mask Selectivity

  • Photoresist Etch Rate
    • SPR 220: 600 A/min
    • Thermal oxide/HTO: unknown

Side Profile

Trench

Running recipe 4 for 20 minutes with 3 µm of SPR 220 on a silicon wafer with our standard DRIE characterization mask can produce a profile like this. The minimum trench size is 0.24 µm.

Scallop

  • 80 nm wide X 300 nm tall

Undercut

  • 225 nm

Grassing

An example of grassing can be seen below. This can happen if there is too much exposed area (>25%) on the mask.

Limitations

Etch Length

Feature Size

Aspect ratio

Open area

Multi-step etching

  • Multi-step processing (i.e. running two or more etches with overlapping features) with the Bosch process is known to cause undesirable results. Please contact the tool engineers if you wish to run such a process so we can help reduce or eliminate issues.

Qualification

Currently Recipe 4 is not routinely qualified.