Tempress S2T3 - Nitride-HTO 6"

From LNF Wiki
Revision as of 19:45, 25 September 2025 by Beach (talk | contribs)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Jump to navigation Jump to search
Tempress S2T3 - Nitride-HTO 6"
30091.jpg
Equipment Details
Technology LPCVD
Materials Restriction CMOS Clean
Sample Size 150mm
Gases Used N2, SiH2Cl2, N2O, NH3
Equipment Manual
Overview System Overview
Operating Procedure SOP
Supported Processes Silicon Nitride, HTO
Maintenance Maintenance

The Tempress diffusion system is a modular horizontal furnace designed to process silicon wafers as part of the manufacturing technology of semiconductor, optical, MEMS, and solar devices. HTO (High Temperature Oxide), Nitride, Oxynitride, and Lower Stress Nitride are formed by using a process called LPCVD, Low Pressure Chemical Vapor Deposition. Chemical vapor deposition forms thin films on the surface of a substrate by thermal decomposition and/or reaction of gaseous compounds. The desired material is deposited directly from the gas phase onto the surface of the wafer. The important factors are gas ratio, temperature, and pressure.


Announcements

  • No announcements at this time.

Capabilities

  • Maximum Thickness
    • HTO = 2µm
    • Silicon Nitride = 7000Å
    • Oxynitride = 1µm
    • LSN = 2µm

System overview

Hardware details

  • Maximum Temperature - 900°C
  • N2 - Maximum flow 10 slpm
  • N2 - Maximum flow 1000 sccm
  • SiH2Cl2 - Maximum flow 200 sccm
  • N2O - Maximum flow 500 sccm
  • NH3 - Maximum flow 500 sccm

Substrate requirements

  • Silicon only
  • Can process up to 25, 150 mm (6") wafers
  • Wafer thickness, ~675um for 150mm (6")
All samples must go through the RCA Pre-Furnace clean procedure before being processed in the furnace

Material restrictions

The Tempress S2T3 - Nitride-HTO 6" is designated as a CMOS Clean class tool. Below is a list of approved materials for the tool. Approved means the material is allowed in the tool under normal circumstances. If a material is not listed, please create a helpdesk ticket or email info@lnf.umich.edu for any material requests or questions.


Supported processes

Process details

Characterization data

Standard operating procedure

Checkout procedure

  1. Create a Help desk Ticket requesting training.
  2. A process engineer will schedule a time for initial training. After completing training the user can attempt a checkout session. It may be necessary for some users to participate in more than one training session, prior to attempting check out.
  3. Schedule a checkout session with a tool engineer via the Help desk Ticket system. If this checkout is successful, the engineer will authorize you on the tool.

Maintenance

  • Paddle - cleaned every 3-6µm of accumulated deposition.
  • Boats, and dummy wafers are replaced every 3-6µm of accumulated deposition.
  • Tube is replaced at 100µm of accumulated deposition.